Appreciation post: the 3/16 rod trick for tube sheet welds on a little 12 inch shell
I've been fighting tube sheet welds on small shells for years, always bird nesting or blowing through the top edge. Last week I had a 12 inch shell with 3/4 inch tubes and decided to drop down to 3/16 rod instead of the 1/8 I usually run. I kept the heat at about 95 amps and did a quick stringer around each tube, then came back with a small weave. It took me 20 minutes less per sheet and the x-ray came back clean on the first try. I used to think smaller rod meant slower going, but on that thin sheet it actually sped things up because I wasn't stopping to fix burn-through. Has anyone else tried stepping down a size for tube sheets, or do you stick with the bigger rod and just watch your travel speed?